High-Performance Fiber Properties Table


Fiber Density
(g/cm³)
Tensile Strength
(g/den)
Modulus
(g/den)
Elongation
(%)
Moisture Regain
(%)
LOI
(%)
Thermal k
(W/m·K)
Melting Point
(°C)
Decomp / Char
(°C)
Use Temp
(°C)
Abrasion Cut / Flex Fatigue UV Creep Chemical Resistance
Spectra®Ultra-high-molecular-weight polyethylene 0.97 35–40 900–1400 3–4 0 17–18 0.4–0.5 147–152 N/A 80–100 High Good Moderate Poor Excellent
Kevlar®Para-aramid 1.44 20–26 500–1000 2–4 4–5 28–30 0.04 N/A 425–480 250–300 Very High Very Good Moderate Excellent Good
Alkex®Para-aramid 1.44 20–26 600–875 2.7–3.5 3.5–4.5 28–30 0.04 N/A 427–482 250–300 Very High Very Good Moderate Excellent Good
Technora®HM-HT aramid 1.39 25–28 500–700 3–4 1–3 25–28 0.05 N/A 500 250–350 High Excellent Good Excellent Very Good
Nomex®Meta-aramid 1.38 7–9 120–180 20–30 4–6 28–30 0.04 N/A 370 200–260 Moderate Good Good Good Good
Vectran™Liquid crystal polymer 1.40 26–30 600–900 3–4 0 28 0.05 330 N/A 150–200 Very High Very Good Poor Excellent Very Good
PBO (Zylon®)Poly(p-phenylene-benzobisoxazole) 1.54 40–42 2000–3000 2.5 1–3 65–68 0.06 N/A 650 300–350 High Very Good Poor Excellent Good
PBIPolybenzimidazole 1.30 3–4 50–70 15–20 10–15 41 0.03 N/A 700+ 300–500 Moderate Good Excellent Very Good Very Good
Polyester (HT PET)High-tenacity polyester 1.38 7–9 150–200 12–20 0.3–0.4 20–22 0.15 255–265 N/A 120–160 Good Good Excellent Very Good Good
Nylon 6,6Polyamide 6,6 1.14 8–10 200–300 18–25 3–5 20–22 0.25 255–265 N/A 90–140 Very High Excellent Moderate Moderate Good
Carbon FiberPAN-based carbon fiber 1.75–1.95 25–45 2000–3500 1–2 0 N/A 5–20 N/A >3000 400+ Moderate Poor Excellent Excellent Excellent
E-Glass FiberElectrical-grade fiberglass 2.55 12–16 700–900 4–5 0 N/A 1.0 850 N/A 400–500 Moderate Poor Excellent Excellent Excellent
Disclaimer: Values represent typical published ranges and may vary by fiber grade and test method.